II.1.2. Preparation of the Cu-Co-Rh / Zn-La catalysts - CoCuRhZnLa-CM



The ZnO-La2O3 support was prepared in the same way like CoCuZnLa-CM but with little different.
After calcination catalyst was prepared by incipient wetness impregnation at room temperature. 5 ml of aqueous solution containing the necessary amount of Co(NO3)2*6H2O, Cu(NO3)2*6H2O and rhodium (III) chloride trihydrate were used for impregnation 2.085 g of support. The impregnated sample was dried at 80 °C overnight and then calcined at 350 °C for 4 h.
3 g of 15% Cu – 15% Co – 0,5% Rh / 90% ZnO – 10% La2O3 catalyst were prepared.